Analysis of Causes for Corrosion of Circulating Water Pump Shafts in Nuclear Power Plants and Repair Techniques
Release time:
2021-10-21 13:47
Tang Huipeng Su Zejun Zhao Baoqian
(CGN Nuclear Power Operation Co., Ltd. Overhaul Center, Shenzhen, Guangdong; 518000)
Abstract: Through the analysis of the corrosion resistance and pitting corrosion resistance of the pump shaft selection materials for the circulating water pump of a nuclear power unit in Daya Bay, it is found that the pump shaft material itself has low corrosion resistance and pitting resistance. The composition of the attachment on the surface of the pump shaft was analyzed and found to contain pitting sensitive ion chloride ions, which could lock the cause of the pitting corrosion of the pump shaft. Through the analysis of the design and assembly structure of the pump shaft, the way for the chloride-containing medium to enter the gap of the pump shaft is found. According to the reasons for the corrosion of the pump shaft, the repair and anti-corrosion measures of the pump shaft were formulated to restore the normal use of the pump shaft and avoid the subsequent continued corrosion of the pump shaft.
Chinese Library Classification Number: TH311 Document Identification Code: A
introduction
Nuclear power plant circulating water system (CRF) circulating water pump mainly provides cooling sea water for condenser and other conventional island equipment. The pump transports seawater to the titanium tube of the condenser to take away the heat, and then returns to the sea from the outlet chamber and drain. Each unit is designed with 2 circulating water pumps, each providing 50% of the circulating water flow. If any one of the CRF pumps fails and stops the pump, it will directly reduce the power of the unit by about 50%, which has a huge impact and is a key sensitive equipment in a nuclear power plant.
1 Device defect description
On December 14, 2013, during the 11th round of overhaul of a nuclear power unit in Daya Bay, during the preventive random inspection and full inspection of the No. 1 circulating water pump, it was found that the shaft journal of the pump shaft and the packing shaft sleeve was corroded with a width of about 100 mm. The appearance of the corrosion zone is dense small pits. The largest pitting pit in the corrosion zone is about 12 mm, and the deepest pitting depth is about 7 mm, as shown in Figure 1.
In October 2015, during the 13th round of overhaul of another unit, during the full inspection of two circulating water pumps, it was found that there were sporadic minor corrosion on the journal surface of the pump shaft and the packing shaft sleeve installation position, as shown in Figure 2. Show. There are about 5 slight corrosion pits on the surface of the No. 1 pump shaft, the largest pit diameter is about 4 mm, and the deepest pit depth is about 2 mm; shaft head. There is slight corrosion near the sealing surface of the ring, and the depth is less than 1mm, which does not affect the sealing surface of the 0-ring. The surface condition of the No. 2 pump shaft is slightly better, with only minor pitting and pitting, and the depth is less than 0.5 mm, but there is slight corrosion of the entire ring near the 0-ring seal of the shaft head. The deepest corrosion depth is about 2 mm, which may affect the 0-ring sealing surface .
During the on-site disassembly process, it was found that a large amount of mushy dirt covered the surface of the pump shaft in the gap between the packing shaft sleeve and the pump shaft. The corrosion of the pump shaft will directly affect the strength of the pump shaft. When the corrosion is severe to a certain extent, it may cause the pump shaft to break during operation and cause the pump to be unusable.

Figure 1 Pitting diagram on the surface of the pump shaft of the No. 1 circulating water pump

Figure 2 Local slight pitting of the pump shaft
2 Operating conditions of the pump set
2.1 Pump set performance parameters
The circulating water pump of the nuclear power plant is a large single-stage vertical centrifugal pump with a cement volute. The performance parameters of the pump are shown in Table 1.
2.2 Pump shaft material performance
The pump shaft material is X20Crl3 (NF EN10088 -3), which is martensitic stainless steel. The chemical composition is shown in Table 2, and the mechanical properties are shown in Table 3.
3 cause analysis
3.1 Analysis of corrosion resistance performance of pump shaft selection materials
The corrosion resistance of steel increases with the increase of Cr content. Generally, Fe-Cr alloys with a Cr content of more than 12% have certain corrosion resistance, commonly known as stainless steel. The Cr content of X2OCrl3 martensitic stainless steel is about 13%, and the maximum pitting resistance equivalent value of the material is calculated according to the pitting equivalent value calculation formula PRE -1 x%Cr + 3.3 x%Mo + 16 x%N = 14 Compared with common austenitic stainless steel 316 (PRE = 24) and common duplex stainless steel 2205 (PRE = 35), it can be seen that X20Crl3 has lower pitting resistance. However, the material can obtain good cutting performance after degrading and softening treatment, and can obtain higher strength and hardness after quenching and tempering treatment, and it is cost-effective. It is often used in shaft parts of conventional equipment.
3.2 Pitting mechanism of pump shaft
The pump shaft material has certain corrosion resistance, but it is prone to pitting corrosion in the medium containing corrosive halogen ions (such as chloride ions), also known as pitting corrosion. Pitting corrosion is one of the main forms of corrosion of this type of stainless steel. Figure, the schematic diagram of the pitting corrosion of the pump shaft is shown in Figure 3. Refer to this type of stainless steel point
According to the latest research information on corrosion mechanism, it is analyzed that: due to various minor defects (such as strain, abrasion, inclusion, unevenness, dislocation "outcrops", etc.) on the surface of the pump shaft, the passivation film at the defect site is relatively fragile. When exposed to aggressive chloride ions, the cations in the passivation film easily react with chloride ions to form soluble chlorides, and the partial passivation film is destroyed. This is the inducing stage of pitting corrosion. The damaged corrosion point becomes the activated anode, and the surrounding area becomes the cathode area. Because the anode area is small, the corrosion current density is large, and the dissolution rate is fast, pitting nuclei are quickly formed on the metal surface. At the same time, the pitting area will also form battery corrosion with a difference in oxygen concentration. Because oxygen at the bottom of the pitting hole is not easy to replenish, the result of lack of oxygen makes the metal decomposition reaction MTM++e\There is a higher concentration of oxygen around the hole, and A reduction reaction occurs O2 +2H2O+4e--> 4OH-, so the surrounding area of the hole is protected from corrosion, and the pitting corrosion in the hypoxic area at the bottom of the hole continues to expand and deepen. The actual corrosion morphology on the surface of the pump shaft is that the pitting pit has a small diameter and a deep depth, which is completely consistent with the aforementioned analysis.

Figure 5 Dirt on the surface of the pump shaft
3.3 Pump shaft assembly structure and source analysis of corrosive media
The circulating water pump is a vertical single-stage centrifugal pump. The upper part of the pump shaft is connected with the gearbox through a coupling, and the lower part is directly connected with the impeller. Its function is to transfer the rotating mechanical energy of the gearbox to the impeller and drive the impeller to rotate and do work.

Figure 4 Schematic diagram of pump shaft assembly and corrosion area

Figure 3 Schematic diagram of pump shaft pitting
As shown in Figure 4, the packing shaft sleeve, protective sleeve, impeller, and deflector are installed from top to bottom on the outside of the pump shaft, and the joint parts of each component are installed. Ring seals (total of 3 0-rings) form a hermetic protection for the pump shaft to prevent the external medium (sea water or packing flushing water) from directly contacting the pump shaft. The top of the packing bushing and the matching position of the pump shaft are not designed with a type 0 sealing ring, because this place is higher than the normal water level of packing leakage, and no medium enters the packing bushing from this place under normal working conditions. The packing shaft sleeve and the pump shaft are in clearance fit, and the mating surfaces are at the upper and lower ends of the packing shaft sleeve. The upper end is designed with a diameter clearance value of Q 018 -0. 143 mm, and the lower end is designed with a diameter clearance value of 0.062 ~ 0. 208 mm; The middle section of the packing sleeve is a non-matching surface, and the clearance with the pump shaft is about 1 mm. The corrosion position of the pump shaft is about 100 mm in the lowest part of the middle non-matching shaft section. It can be seen from the drawing that the pump shaft is not designed to be in direct contact with the seawater medium, so the manufacturer chooses the material X20Crl3o with lower corrosion resistance.
After the packing shaft sleeve was disassembled on site, it was found that there was mushy dirt in the matching gap between the packing shaft sleeve and the pump shaft (as shown in Figure 5), and three inspections were performed on site. The sealing condition of the ring is normal. Inquiring about the relevant historical records of the nuclear power plant, it was found that the circulating water pump had been flooded in the pump pit. The reason was that the sewage tank water level increased due to the failure of the sewage pump of the pump station and the sewage was poured back into the circulating water pump pit through the sewage pipe of the circulating pump. It has been submerged to the rotating oil tank above the packing sleeve. At this time, sewage may seep into the gap between the packing sleeve and the pump shaft through the gap between the top of the packing sleeve and the pump shaft. In addition, the moisture and salt content of the moist environment at the seaside of the pumping station is relatively high, and the salty moisture in the air can also directly penetrate into the packing shaft sleeve through the gap at the top of the packing shaft sleeve.
3.4 Laboratory analysis of the medium composition on the surface of the pump shaft
|
Table 4 |
Chloride ion content table |
|
Medium source |
Chloride ion content/ppm |
|
No. 2 pump No. 2 |
1000 |
|
No. 1 pump No. 1 pump |
3430 |
|
No. 1 pump No. 2 pump |
3900 |
|
Packing flushing water (SDA water) |
30 |
|
Pump chamber sea water |
19000 |
According to the test results, it is confirmed that the medium on the surface of the pump shaft contains highly corrosive chloride ions, and the degree of corrosion on the surface of the pump shaft is directly related to the chloride ion content. The higher the chloride ion content, the more serious the corrosion, and the lower the chloride ion content, the slight corrosion. Or no corrosion.
3.5 Analysis of Causes of Pump Shaft Corrosion
The direct cause: The external chloride-containing medium accidentally enters the packing shaft sleeve through the gap at the top of the packing shaft sleeve, soaking the pump shaft for a long time, resulting in pitting corrosion of the pump shaft.
The root cause: There is an opening gap between the top of the original design packing sleeve and the fitting of the pump shaft, and no sealing ring is designed. During the commissioning period, sewage accidentally flooded the pump pit, and the tidal water near the pump station contains chloride ions, which can penetrate into the shaft sleeve through the gap at the top of the shaft sleeve, forming a pitting environment.
Contributing factor: The pump shaft material X20Crl3 has low resistance to chloride ion pitting.
The cause factor analysis diagram is shown in Figure 6.
4 Pump shaft repair
After calculating that the strength of the pump shaft still meets the operating requirements, by drawing on historical experience and repeated simulation tests, we independently developed a corrosion pump shaft repair technology, and quickly completed the pump shaft repair and restored the pump shaft to be usable.
4.1 Autonomous repair technology
1) Determine the repair area, and remove the corroded layer of the repaired area on the pump shaft by turning. The repaired area should cover the entire corroded part. The turning of the corroded layer requires that the corroded layer be completely removed. Since the depth of turning may affect the strength of the pump shaft, it is necessary to determine the turning depth based on the strength of the pump shaft and the depth of corrosion. After turning to remove the corrosion layer, the shaft diameter after turning is still larger than the smallest shaft diameter of the entire pump shaft. It can be determined that the strength of the pump shaft after turning still meets the pump operation requirements.
In addition, after turning to remove the corrosion layer, the transition fillet of the starting and ending points of turning is cut to avoid stress concentration.
2) The thread is further turned in the repair area to form a threaded area, and the thread pitch is 1.0 mmo
The purpose of turning the threaded area is to increase the adhesion area of the metal repair agent, increase the surface roughness of the repair area, and improve the adhesion and bonding force of the repair agent. After turning to form the threaded area, the starting point and the end point of turning are turned and the transition fillet is made to avoid stress concentration.
3) Apply metal repair agent to the cleaned area of turning. The selection of metal repair agent requires fine particle size, thin viscosity, strong corrosion resistance, and can reach maximum strength within 24 hours. After hardening, the hardness is moderate, and the toughness is good, which is convenient Turning. After trying out various types of metal repair agent, Belzona 1321 metal repair agent was finally selected.

Figure 6 Time sequence and cause factor analysis diagram
During the full inspection of the three circulating water pumps, samples of dirt on the surface of the pump shafts were collected and analyzed for chloride ion content. The results are shown in Table 4.
references
[1 ] NF EN10088 - 3 - 2005. Stainless steels-Part 3: Technical delivery conditions for semifinished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes.
[2] Ye Chao, Du Nan. Zhao Qing, et al. Pitting corrosion behavior of stainless steel and progress in research methods [J]. Corrosion and Protection, 2014, 35 (3): 271 -276.
[3] Shi Lin, Zheng Zhijun, Gao Yan. Pitting corrosion mechanism and research methods of stainless steel[J]. Materials Guide, 2015, 29 (12); 79 -85.
(Edited by Tang Lili of this article) (Received 2019-07-10)